FixForge › Vintage › Cast Iron Electrolysis Tank Setup

Cast Iron Electrolysis Tank Setup

Electrolysis lifts rust and old build-up off cast iron without removing sound metal, which is why collectors use it on pans worth keeping. No cookware maker or extension service publishes a method. The two standard references are The Cast Iron Collector and the Wagner and Griswold Society, and they disagree on several points. This page gives both and says where they part.

Last Updated: November 2026

Illustrated before-and-after diagram of a cast iron skillet showing rust and a seasoned surface
Illustrated diagram — not a photo of an actual pan. Yours may vary.

Fast Answer

Fill a plastic tub with water and dissolve 1 tablespoon of washing soda per gallon. Hang a piece of scrap iron or steel in the water as the anode. Hang the pan so it does not touch the anode. Clip the charger's negative (black) lead to the pan and the positive (red) lead to the anode. Use a manual battery charger, work outdoors or with ventilation because the bubbles are flammable hydrogen, and switch off before reaching in.

Washing soda, not baking soda

1 tablespoon per gallon. The Cast Iron Collector allows 1 to 2.

Black lead on the pan

Both guides agree: negative to the piece being cleaned, positive to the sacrificial anode.

Manual charger

An automatic charger reads the tank as a charged battery and shuts itself off.

Ventilate

The process gives off hydrogen. Keep it away from pilot lights and never seal the tank.

What You Need

ItemThe Cast Iron CollectorWagner and Griswold Society
ContainerPlastic, able to hold eight or more gallons of waterMust be non-metallic
ElectrolyteArm & Hammer Super Washing Soda, not baking sodaSodium carbonate (washing soda)
Amount1 to 2 tablespoons per gallon of water1 tablespoon per gallon
AnodeIron or steel: scrap sheet steel, rebar, mower bladesJust about anything metallic; it calls stainless steel the ultimate
ChargerManual, or with a manual mode. The author uses a 2-amp/10-amp switchable unitA 12-volt charger capable of 35 to 40 amps is ideal; 6-volt or trickle chargers will be extremely slow
TimeA couple of sessions of about 8 hours eachCheck after an hour or so; 6 or 8 hours

The two agree on the essentials: a plastic container, washing soda at about a tablespoon per gallon, and a 12-volt battery charger. They differ on how much current is useful. A small charger works; it is just slower.

Why the Charger Has to Be Manual

Modern automatic chargers look for a battery before they deliver current. The Cast Iron Collector explains the problem: an automatic charger will see the electrolysis tank as a charged battery and shut itself down. It gives three ways around it: a charger that is manual or has a manual mode, an automatic charger connected to a 12-volt car battery that in turn feeds the tank, or a constant-current DC power supply.

Setting It Up

  1. Put the plastic container somewhere outdoors or well ventilated, on a surface that can get wet.
  2. Fill it with water and stir in washing soda at 1 tablespoon per gallon until it dissolves.
  3. Suspend the anode in the water at one side. Part of it must stay above the surface so the clamp connects to dry metal.
  4. Suspend the pan in the water so that it faces the anode and does not touch it. If the pan and anode touch, you have a short circuit.
  5. With the charger unplugged, clip the negative (black) lead to the pan and the positive (red) lead to the anode.
  6. Plug in and switch on. Fine bubbles should begin rising from the pan.
  7. Switch off and unplug before you adjust or remove anything.

Polarity is the one thing you must not get backwards. The Wagner and Griswold Society puts it in capitals: the black negative clamp must be attached to the part to be cleaned. Reversed, the pan becomes the sacrificial piece and is eaten away instead of cleaned.

Line of Sight

The Cast Iron Collector describes electrolysis as largely a line-of-sight process. The surface facing the anode cleans first and fastest. Turn the pan partway through so that the bottom, the sides and the handle each get a turn facing the anode, or use more than one anode around the tank.

Hydrogen and Electrical Safety

  • The Cast Iron Collector: the process produces potentially flammable hydrogen gas, so work in a well-ventilated area or outdoors.
  • The Wagner and Griswold Society: the bubbles are pure hydrogen and extremely flammable. Do not set the tank up by an open pilot light, and make sure there is ventilation.
  • Do not cover the tank with a tight lid, which would trap the gas.
  • Always turn off the power before putting your hands in the water or moving the clamps.

A garage with a gas water heater or furnace is a poor place for this. Outdoors under cover is better.

The Stainless Steel Anode Question

The sources contradict each other here, and none of them is an authority on chemical safety.

  • The Wagner and Griswold Society recommends stainless steel as the best anode because it lasts.
  • Other hobby guides warn that a stainless anode releases chromium compounds, including hexavalent chromium, into the bath.
  • The Cast Iron Collector reports that warning and disputes it, saying the concern comes from industrial electroplating and does not apply at these voltages and temperatures.

No safety data sheet, government source or manufacturer settles the question. Plain iron or mild steel works, costs nothing and raises no such doubt, so that is the simple choice. The anode will rust and foul as it works; pull it and scrub it clean when the bubbling slows.

Which Pieces Should Not Go in the Tank

The Cast Iron Collector says electrolysis should only be used to clean bare cast iron ware. Its specific cautions:

  • Chrome or nickel plated pieces may or may not be adversely affected. Elsewhere it says electrolysis could remove plating, especially where adhesion is already compromised.
  • Enamelled cast iron may have its coating compromised.
  • Aluminium will dissolve.

If you are not sure what you have, identify it first: Identify and Date a Cast Iron Skillet Before Restoring.

When It Is Done

The rust turns to a loose black film. Take the pan out, scrub it under running water with a stiff brush or steel wool, and look. If rust remains, put it back with a different face toward the anode. When it is clean it is bare iron, and it will start rusting again almost immediately, so dry it with heat and season it straight away: Re-Seasoning Cast Iron After Stripping.

On disposing of the used solution the two guides disagree again. One pours it out in the yard; the other cautions against contaminating soil near vegetable gardens. Neither cites a regulation. Check your local rules for household chemical disposal.

Supplies reference

ItemDetailNotes
Washing soda (sodium carbonate)1 tablespoon per gallon of waterArm & Hammer Super Washing Soda is the product named. Not baking soda.
Manual 12-volt battery chargerManual, or with a manual modeAutomatic-only chargers shut off.
Plastic containerEight gallons or moreNever metal.
Scrap iron or mild steelThe sacrificial anodeRebar, sheet steel or a mower blade.

Sources

Ratios, temperatures, times, dates and safety statements on this page come from the sources below, and the text names which source each comes from. Manufacturer, university extension, government and safety-data-sheet sources are used where they exist; where a point rests on collector or test-kitchen references only, the text says so. Plain handling steps are general practice.

Manual 12V Battery Charger

Must be manual or have a manual mode. An automatic-only charger will not run an electrolysis tank.

Check Price on Amazon →

As an Amazon Associate, FixForge earns from qualifying purchases.

Arm & Hammer Super Washing Soda

Sodium carbonate, the electrolyte both collector guides specify. Baking soda is a different chemical.

Check Price on Amazon →

As an Amazon Associate, FixForge earns from qualifying purchases.